View Single Post
  #4   Report Post  
Leon McAtee
 
Posts: n/a
Default Aluminum casting problem

"Smelly Belly" wrote in message ...
check your gating system. Are you using a pressurized or non-pressurized
gating system? What's your ratio for downsprue: runner : ingate?

Tricks to help can include:
* reduce pouring height
* put bigger well at bottom of downsprue
* go to non-pressurized system
* put traps at end of runners
* dog legs in runners/gates
* minimize turbulance and metal veloceties in gating system

You can get some good books/training courses at the following:
http://www.afsinc.org


Thanks for the link. I suspect the last parameter is the one giving
me the problems. My ingate is quite small due to the thiness of the
casting. Metal velocity at that point is probably high. I also was
trying to keep the hydrostatic pressure high to help fill. My first
attempt only filled partialy - but had no sand includions.